SA-213/SA-213M Specification for seamless Ferritic Alloy steel boiler, Superheater and heat exchanger tubes 


Delivery Condition: Normalized and Tempered
Inspections and Tests Performed: Chemical Composition Inspection, Mechanical Properties Test(Tensile Strength, Yield Strength, Elongation, Flaring, Flattening, Bending, Hardness, Impact Test), Surface and Dimension Test, No-destructive Test, Hydrostatic Test.
Surface treatment: Oil-dip, Varnish, Passivation, Phosphating, Shot Blasting

Inner packing: Caps on two ends of every pipe

Package: bare packing/bundle packing/wooden carton packing.

Size Tolerance

Tube Kinds

SA213 ODD

SA213 ThicknessS

ODmm

OD Tolerancemm

ODmm

Thickness Tolerancemm

Hot Rolled

101.6

+0.4-0.8

76168.3

+28%0

>101.6168.3

+0.4-1.2

Cold Drawn

<25.4

0.1

38.1

+20%0

25.438.1

0.15

>38.1<50.8

0.2

>38.1

+22%0

50.8<63.5

0.25

63.5<76.2

0.3

76.2101.6

0.38

>101.6190.5

+0.38-0.64

>190.5228.6

+0.38-1.14



Grade

Tensile Strength,Min., ksi[MPa]

Yield Strength,Min., ksi[MPa]

Elongation
in 2 in. or 50 mm,Min., %[Note (1),(2)]

T12

60 [415]

32 [220]

30

T23

74 [510]

58 [400]

20

T91

85 [585]

60 [415]

20

T92

90 [620]

64 [440]

20

T122

90 [620]

58 [400]

20

18Cr-2Mo

60 [415]

40 [275]

20

NOTES:

(1) When standard round 2 in. or 50 mm gage length or smaller proportionally sized specimens with gage length equal to 4D (4

times the diameter) is used, the minimum elongation shall be 22% for all ferritic grades except 18Cr-2Mo, T23 and T91.

(2) For longitudinal strip tests, a deduction from the basic minimum



CHEMICAL REQUIREMENTS FOR FERRITIC STEEL

Composition, %

Grade

Carbon

Manganese

Phosphorus, Max.

Sulfur, Max

 Silicon

Chromium

Molybdenum

Titanium

Vanadium,Min.

Other Elements

T2 [Note (1)]

0.10–0.20

0.30–0.61

0.025

0.025

0.10–0.30

 0.50–0.81

 0.44–0.65

 . . .

 . . .

T5

0.15 max.

0.30–0.60

0.025

0.025

0.50 max.

4.00–6.00

0.45–0.65

. . .

. . .

T5b

0.15 max.

0.30–0.60

0.025

0.025

1.00–2.00

4.00–6.00

0.45–0.65

 . . .

. . .

T5c

0.12 max.

0.30–0.60

0.025

0.025

0.50 max.

4.00–6.00

0.45–0.65

[Note (1)]

 . . .

T9

0.15 max.

0.30–0.60

0.025

0.025

0.25–1.00

8.00–10.00

0.90–1.10

. . .

. . .

T11

0.05 min.–0.15 max.

0.30–0.60

0.025

0.025

0.50–1.00

1.00–1.50

0.44–0.65

 . . .

. . .

T12 [Note (1)]

0.05 min.–0.15 max.

0.30–0.61

0.025

0.025

0.50 max.

0.80–1.25

0.44–0.65

. . .

. . .

T17

0.15–0.25

0.30–0.61

0.025

0.025

0.15–0.35

0.80–1.25

. . .

 . . .

0.15

T21

0.05 min.–0.15 max.

 0.30–0.60

0.025

0.025

0.50 max.

2.65–3.35

0.80–1.06

 . . .

. . .

T22

0.05 min.–0.15 max.

0.30–0.60

0.025

0.025

0.50 max.

1.90–2.60

0.87–1.13

. . .

 . . .

T23

0.04–0.10

0.10–0.60

0.03

0.01

0.50 max.

1.90–2.60

0.05–0.30

 . . .

0.20–0.30

W 1.451.75
Cb 0.02
0.08
B 0.0005
0.006
N 0.030 max.
Al 0.030 max.

T91

0.08–0.12

0.30–0.60

0.02

0.01

0.20–0.50

8.00–9.50

0.85–1.05

. . .

0.18–0.25

Cb 0.060.1
N 0.030
0.070
Ni 0.40 max.
Al 0.04 max.

T92

0.07–0.13

0.30–0.60

0.02

0.01

0.50 max.

8.50–9.50

0.30–0.60

. . .

0.15–0.25

W 1.52.00
Cb 0.04
0.09
B 0.001
0.006
N 0.03
0.07
Ni 0.40 max.
Al 0.04 max.

T122

0.07–0.14

0.70 max.

0.02

0.01

0.50 max.

10.00–12.50

0.25–0.60

. . .

0.15–0.30

W 1.502.50
Cu 0.30
1.70
Cb 0.04
0.10
B 0.0005
0.005
N 0.040
0.100
Ni 0.50 max.
Al 0.040 max.

18Cr-2Mo

0.025 max.

1.00 max.

0.04

0.03

1.00 max.

17.5–19.5

1.75–2.50

[Note (3)]

 . . .

N max. 0.035
Ni + Cu max. 1.00

NOTES:

(1) It is permissible to order T2 and T12 with 0.045 max. Sulfur.

(2) Grade T5c shall have a titanium content of not less than four times the carbon content and not more than 0.70%.

(3) Grade 18Cr-2Mo shall have Ti + Cb p 0.20 + 4 (C + N) min., 0.80 max.